Home / Tutorial / What Is Welding Electrode Redrying and When Is It Necessary?

What Is Welding Electrode Redrying and When Is It Necessary?

Redrying of welding electrodes is the process of re-drying electrodes using a specialized oven at a specific temperature and for a set duration, in order to reduce the moisture absorbed by the flux coating. 

This process is important for maintaining electrode performance and reducing the risk of welding defects, particularly when using low-hydrogen electrodes.

In SMAW welding, the condition of the electrode is one of the factors that influence the quality of the weld joint. Therefore, redrying must be performed in accordance with the manufacturer's recommendations and the technical requirements of the work.

Redrying is the process of reheating welding electrodes in a controlled manner to reduce the moisture content in the electrode's protective coating or flux.

This process differs from holding, even though both utilize electrode heating equipment.

Aspect

Redrying

Holding

Objective

Reducing absorbed moisture

Keeping the electrodes dry

Temperature

In accordance with re-drying specifications

Generally lower

Time

A specific duration

During temporary storage

Equipment

Redrying oven

Holding oven

Redrying helps restore electrodes that have absorbed moisture, while holding helps prevent them from reabsorbing moisture before they are used.

Why Do Welding Electrodes Need to Be Re-dried?

The flux coating on SMAW electrodes can absorb moisture from the air during storage or while in use in the field. This moisture can serve as a source of hydrogen within the weld metal.

According to Kobe Steel, Ltd., in its publication *Welding of Medium/High Carbon Steels and Special Steels*, re-drying is necessary when the moisture content in low-hydrogen electrodes reaches approximately 0.3–0.5%, depending on the type of electrode.

Excessive humidity levels can increase the risk of:

  • Porosity in weld metal.

  • Hydrogen-induced cracking.

  • Instability of the welding arc.

  • Reduced consistency in welding results.

  • Increased need for weld joint repairs.

Humidity control is crucial when using low-hydrogen electrodes, particularly for steel construction, pipe welding, and industrial projects with stringent quality requirements.

When Is Redrying of Welding Electrodes Necessary?

Redrying is not always necessary for every electrode before use. The need for it is determined by the type of electrode, storage conditions, history of exposure to the air, and the manufacturer's recommendations.

1. Electrode Exposed to Humid Air

Electrodes left for too long in a high-humidity environment may absorb moisture. Re-drying may be necessary if such conditions exceed the limits specified by the manufacturer.

2. Electrode Packaging Has Been Opened

Once the packaging has been opened, protection against moisture may be reduced. Electrodes must be handled in accordance with the applicable storage requirements and exposure time limits.

3. Exposure Time Limit Exceeded

In industrial projects, low-hydrogen electrodes generally have a specified limit for exposure to open air. If this limit is exceeded, the electrodes must be evaluated before they can be used again.

4. Required by the Welding Procedure

Certain industrial operations mandate the control of electrode conditions—via a Welding Procedure Specification (WPS) or a procedure for managing consumables—to meet quality requirements for welded joints.

What Are the Temperature and Duration for Redrying Welding Electrodes?

The redrying temperature for welding electrodes varies depending on the composition of the flux coating and the specific characteristics of each product. Using an inappropriate temperature can damage the electrode coating and impair welding performance.

The following are the re-drying conditions for several KOBELCO electrodes, based on official product specifications.

KOBELCO Electrodes

Classification

Redrying temperature

Duration

RB-26

E6013

70–100°C

30–60 minutes

LB-26

E7016

300–350°C

30–60 minutes

LB-52

E7016

300–350°C

30–60 minutes

LB-52-18

E7018

300–350°C

30–60 minutes

LB-52U

E7016

300–350°C

30–60 minutes

Source: KOBELCO Welding Handbook, Kobe Steel, Ltd., and technical product specifications from PT Intan Pertiwi Industri.

The data indicates that the RB-26 electrode requires a significantly lower re-drying temperature compared to the LB Series electrodes.

The temperatures and durations in the table apply only to the specified products and cannot be generalized to all electrodes with the same AWS classification.

How to Properly Redry Welding Electrodes

Redrying of electrodes must be performed using a specialized oven with controlled temperature settings.

The following are the general steps for redrying welding electrodes:

  1. Electrode identification. Check the type, classification, and manufacturer's recommendations for re-drying.

  2. Check the physical condition. Ensure that the flux coating is not cracked, peeling, or contaminated.

  3. Prepare an electrode oven. Use an oven with reliable temperature settings and measurement capabilities.

  4. Set the temperature and duration. Follow the product specifications and the applicable heating procedures.

  5. Perform re-drying. Ensure the electrodes are heated evenly.

  6. Transfer to a holding oven. Store the electrodes under the required conditions to prevent the reabsorption of moisture.

For industrial operations, recording temperature, duration, and the redrying history can also assist with quality control and the traceability of consumables.

Mistakes to Avoid During Redrying

Improper re-drying can damage electrodes and cause their performance to deviate from the original specifications.

Some mistakes to avoid include:

  • Using a temperature that exceeds the manufacturer's recommendations.

  • Equalizing the redrying temperature for all types of electrodes.

  • Using an oven that lacks adequate temperature control.

  • Performing repeated drying cycles without regard for the permitted limits.

  • Reusing electrodes with a damaged flux coating.

  • Applying a low-hydrogen redrying temperature to cellulosic electrodes.

Cellulosic electrodes require a specific moisture content within their flux coating to support their welding characteristics. Therefore, this type of electrode should not be treated in the same way as low-hydrogen electrodes.

KOBELCO Low-Hydrogen Electrode Recommendations

PT Intan Pertiwi Industri provides a variety of KOBELCO low-hydrogen electrodes to meet industrial welding requirements, including:

  • LB-26 (E7016): for welding steel that requires hydrogen control.

  • LB-52 (E7016): for various structural welding applications.

  • LB-52-18 (E7018): for welding applications requiring a low-hydrogen electrode with iron powder in the flux.

  • LB-52U (E7016): designed to support one-sided welding, including root passes on pipes.

Proper redrying, combined with the selection of electrodes suited to the material and the welding procedure, helps maintain consistent quality in welded joints.

Frequently Asked Questions (FAQ) Regarding the Redrying of Welding Electrodes

Do all welding electrodes need to be re-dried?

No. The need for redrying depends on the type of electrode, storage conditions, and the manufacturer's recommendations.

Not necessarily. Electrodes in packaging that remains well-protected can be used without redrying, provided this is permitted by the manufacturer and the project procedures.

There is no single universal limit that applies to all electrodes. The number of times an electrode may be re-dried must be in accordance with the manufacturer’s specifications and the applicable requirements for consumable control.

Not necessarily. For example, the KOBELCO RB-26 (E6013) has a redrying temperature of 70–100°C, whereas the LB-52-18 (E7018) requires a temperature of 300–350°C for redrying.

Redrying helps reduce one of the sources of hydrogen in welding, thereby lowering the risk of hydrogen-induced cracking. However, other factors—such as the material, stress, temperature, and welding procedures—must still be controlled.

Conclusion

Redrying welding electrodes is a crucial aspect of quality control for consumables, particularly when using low-hydrogen electrodes. The temperature, duration, and conditions for redrying must adhere to the manufacturer's specifications to ensure that the electrode's characteristics are maintained.

PT Intan Pertiwi Industri offers a wide selection of KOBELCO welding electrodes to support industrial welding requirements with consistent quality standards.

Contact us for product information and technical support tailored to your welding needs.

Other Articles

ISO certificate

ISO 9001:2015

ISO 14001:2015

© 2026, PT. Intan Pertiwi Industri | All Rights Reserved.

Social Sticky
IndonesianEnglish